Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Ultramid® A3EG7 - PA66-GF35 - BASF

Material Data Center offers the following functions for Ultramid® A3EG7:
unit conversion, PDF datasheet print, comparison with other plastics, application examples, snap fit calculation, beam deflection calculation, parameters for material models, CAE Interfaces

Check here, which other Ultramid A datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
材料文字说明
玻璃纤维增强注塑等级, 用于机器零部件和高刚度与尺寸稳定的外壳, 例如灯座外壳、 蒸汽泵、 流体加热器以及电气绝缘零部件。
加工/物理特性干 / 已调节单位Test Standard
ISO数据
熔体体积流动速度, MVR 30 / * cm³/10min ISO 1133
温度 275 / * °C -
载荷 5 / * kg -
模塑收缩率, 平行 0.5 / * % ISO 294-4, 2577
模塑收缩率, 垂直 1.0 / * % ISO 294-4, 2577
喷射温度 195 °C -
机械性能干 / 已调节单位Test Standard
ISO数据
拉伸模量 11500 / 8500 MPa ISO 527
断裂应力 210 / 150 MPa ISO 527
断裂伸长率 3 / 5 % ISO 527
拉伸蠕变模量, 1000h * / 6650 MPa ISO 899-1
无缺口简支梁冲击强度, +23°C 95 / 107 kJ/m² ISO 179/1eU
简支梁冲击强度, -30°C 75 / 77 kJ/m² ISO 179/1eU
简支梁缺口冲击强度, +23°C 14 / 22 kJ/m² ISO 179/1eA
简支梁缺口冲击强度, -30°C 12 / - kJ/m² ISO 179/1eA
热性能干 / 已调节单位Test Standard
ISO数据
熔融温度, 10°C/min 260 / * °C ISO 11357-1/-3
热变形温度, 1.80 MPa 250 / * °C ISO 75-1/-2
热变形温度, 0.45 MPa 260 / * °C ISO 75-1/-2
维卡软化温度, B 250 / * °C ISO 306
线性热膨胀系数, 平行 22 / * E-6/K ISO 11359-1/-2
线性热膨胀系数, 垂直 93 / * E-6/K ISO 11359-1/-2
1.5mm名义厚度时的燃烧性 HB / * class IEC 60695-11-10
测试用试样的厚度 1.6 / * mm -
Yellow Card 现存 是的 / * - -
厚度为h时的燃烧性 HB / * class IEC 60695-11-10
测试用试样的厚度 0.8 / * mm -
Yellow Card 现存 是的 / * - -
燃烧性-氧指数 24 / * % ISO 4589-1/-2
电性能干 / 已调节单位Test Standard
ISO数据
相对介电常数., 100Hz 4.3 / 10.1 - IEC 62631-2-1
相对介电常数., 1MHz 3.8 / 4.5 - IEC 62631-2-1
介质损耗因子, 100Hz 120 / 1570 E-4 IEC 62631-2-1
介质损耗因子, 1MHz 210 / 830 E-4 IEC 62631-2-1
体积电阻率 1E13 / 1E10 Ohm*m IEC 62631-3-1
表面电阻率 * / 1E10 Ohm IEC 62631-3-2
介电强度 39 / 37 kV/mm IEC 60243-1
相对漏电起痕指数 - / 550 - IEC 60112
其它性能干 / 已调节单位Test Standard
吸水性 5 / * % 类似ISO 62
吸湿性 1.6 / * % 类似ISO 62
密度 1410 / - kg/m³ ISO 1183
模塑测量的特殊性能干 / 已调节单位Test Standard
ISO数据
粘数 145 / * cm³/g ISO 307, 1157, 1628
试样制备条件价值单位Test Standard
ISO数据
注塑, 熔体温度 290 °C ISO 294
注塑, 模具温度 80 °C ISO 294
注塑, 注射速度 200 mm/s ISO 294
加工推荐(注塑)价值单位Test Standard
预干燥-温度 80 °C -
预干燥-时间 4 h -
加工湿度 ≤0.15 % -
注塑熔体温度 280 - 300 °C -
模具温度 80 - 90 °C -
函数
粘度-剪切速度 , Ultramid® A3EG7, PA66-GF35, BASF
剪切应力-剪切速度 , Ultramid® A3EG7, PA66-GF35, BASF
动态剪切模量-温度 , Ultramid® A3EG7 (烘干), PA66-GF35, BASF
动态剪切模量-温度 , Ultramid® A3EG7 (状况), PA66-GF35, BASF
应力-应变.  , Ultramid® A3EG7 (烘干), PA66-GF35, BASF
应力-应变.  , Ultramid® A3EG7 (状况), PA66-GF35, BASF
正割模量-应变.  , Ultramid® A3EG7 (烘干), PA66-GF35, BASF
正割模量-应变.  , Ultramid® A3EG7 (状况), PA66-GF35, BASF
应力-应变(等时的) 23°C, Ultramid® A3EG7 (状况), PA66-GF35, BASF
蠕变模量-时间. 23°C, Ultramid® A3EG7 (状况), PA66-GF35, BASF
蠕变曲线 23°C, Ultramid® A3EG7 (状况), PA66-GF35, BASF
应力-应变(等时的) 60°C, Ultramid® A3EG7 (烘干), PA66-GF35, BASF
蠕变模量-时间. 60°C, Ultramid® A3EG7 (烘干), PA66-GF35, BASF
蠕变曲线 60°C, Ultramid® A3EG7 (烘干), PA66-GF35, BASF
应力-应变(等时的) 90°C, Ultramid® A3EG7 (烘干), PA66-GF35, BASF
蠕变模量-时间. 90°C, Ultramid® A3EG7 (烘干), PA66-GF35, BASF
蠕变曲线 90°C, Ultramid® A3EG7 (烘干), PA66-GF35, BASF
应力-应变(等时的) 120°C, Ultramid® A3EG7 (烘干), PA66-GF35, BASF
蠕变模量-时间. 120°C, Ultramid® A3EG7 (烘干), PA66-GF35, BASF
蠕变曲线 120°C, Ultramid® A3EG7 (烘干), PA66-GF35, BASF
应力-应变(等时的) 140°C, Ultramid® A3EG7 (烘干), PA66-GF35, BASF
蠕变模量-时间. 140°C, Ultramid® A3EG7 (烘干), PA66-GF35, BASF
蠕变曲线 140°C, Ultramid® A3EG7 (烘干), PA66-GF35, BASF
比容-温度(pvT) , Ultramid® A3EG7, PA66-GF35, BASF
拉伸模量-温度 , Ultramid® A3EG7 (烘干), PA66-GF35, BASF
拉伸模量-温度 , Ultramid® A3EG7 (状况), PA66-GF35, BASF
典型数据
加工方法
注塑
供货形式
粒料
添加剂
润滑剂, 脱模助剂
特殊性能
经热稳处理的/耐热的
地区供应
其他信息
注塑成型
PREPROCESSING
Pre/Post-processing, max. allowed water content: .15 %
Pre/Post-processing, Pre-drying, Temperature: 80 °C
Pre/Post-processing, Pre-drying, Time: 4 h

PROCESSING
injection molding, Melt temperature, range: 280 - 300 °C
injection molding, Melt temperature, recommended: 290 °C
injection molding, Mold temperature, range: 80 - 90 °C
injection molding, Mold temperature, recommended: 80 °C
injection molding, Dwell time, thermoplastics: 10 min
耐化学性
酸类
醋酸 (5g/100g) (23°C)
权利义务的法律声明
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com